Table 6 UHPC mix design properties for closure joint

From: Modeling life expectancy and cost effectiveness for UHPC bridge retrofitting techniques

Material

1% steel Fiber Mix Quantity kg/m3

 Cement

707

 Slag

354

 Silica Fumes

118

 Water

236

 w/b

0.2

 Sand

1179

 Steel Fibers

79

 Superplasticizer

13.5

Properties

1% Steel Fiber Mix

 Compressive Strength, Mpa

128.9

 Flexural Strength, Mpa

14.3

 Direct Tensile Strength, Mpa

4.83

 Water Cement Ratio

0.25